技术参数
性能项目 试验条件[状态] 测试方法 测试数据 数据单位
基本性能密度ASTM D-7921.42
物理性能吸水量浸泡均衡点+73℉(+23℃)ASTM D-5700.90%
吸水量Equil.50%R.h.+73℉(+23℃)ASTM D-5700.22%
吸水量24hrs浸泡+73℉(+23℃)ASTM D-5700.25%
热性能热变形温度264psiASTM D-648277
热变形温度66psiASTM D-648342
热变形温度0.5MPaASTM D-648172
热变形温度1.8MPaASTM D-648136
熔点ASTM D-2133175
熔点ASTM D-2133347
线性热膨胀系数-40 to +29℃ASTM D-69610.410-5m/m.℃
线性热膨胀系数-40 to +85℉ASTM D-6965.810-5in/in.℉
线性热膨胀系数+104 to +150℃ASTM D-69614.910-5m/m.℃
线性热膨胀系数+220 to +300℉ASTM D-6968.310-5in/in.°F
线性热膨胀系数+140 to +220℉ASTM D-6967.610-5in/in.°F
线性热膨胀系数+60 to +104℃ASTM D-69613.710-5m/m.℃
线性热膨胀系数+29 to +60℃ASTM D-69612.210-5m/m.℃
线性热膨胀系数+85 to +140℉ASTM D-6966.810-5in/in.℉
热传导系数2.6BTU-in/hr
热传导系数0.37W/mk
可燃烧性UL-9494HB
机械性能洛氏硬度ASTM D-785M94,R120
IZOD冲击强度40℃ASDM D-25664.1j/m
IZOD冲击强度+23℃ASTM D-25674.7j/m
IZOD冲击强度+73℉ASDM D-2561.4ft.lb/in
IZOD冲击强度-40℉ASDM D-2561.2ft.lb/in
挠曲系数+70℃在25℃下1585MPa
挠曲系数+23℃在25℃下2830MPa
挠曲系数-55℃在25℃下3930MPa
挠曲系数+158℉在25℃下230MPsi
挠曲系数+212℉在25℃下90MPsi
挠曲系数+73℉在25℃下410MPsi
挠曲系数-68℉在25℃下570MPsi
挠曲系数+122℃在25℃下620MPa
伸张强度+158℉ASTM D-6386.9MPsi
伸张强度+70℃ASTM D-63847.5MPa
伸张强度+100℃ASTM D-63835.9MPa
伸张强度+212℉ASTM D-6385.2MPsi
伸张强度-68℉ASTM D-63814.7MPsi
伸张强度-55℃ASTM D-638101MPa
伸张强度+122℃ASTM D-63826.2MPa
伸张强度+250℉ASTM D-6383.8MPsi
伸张强度+73℉ASTM D-63810.0MPsi
伸张强度+23℃ASTM D-63868.9MPa
压缩应力+73℉@1%Def.ASTM D-6955.2MPsi
压缩应力+23℃@10%Def.ASTM D-695124MPa
压缩应力+23℃@1%Def.ASTM D-69535.9MPa
压缩应力+73℉@10%Def.ASTM D-69518.0MPsi
断裂时之拉力伸张度+73℉(+23℃)ASTM D-63840%
断裂时之拉力伸张度+250℉(+122℃)ASTM D-638>260%
断裂时之拉力伸张度+212℉(+100℃)ASTM D-638>260%
断裂时之拉力伸张度-68℉(-55℃)ASTM D-63813%
断裂时之拉力伸张度+158℉(+70℃)ASTM D-638220%
断裂时之拉力伸张度+250℉(+122℃)ASTM D-638>260%
弹性系数+23℃ASTM D-6383100MPa
弹性系数+73℉ASTM D-638450MPsi
剪力+23℃ASTM D-73265.5MPa
剪力+73℉ASTM D-7329.5MPsi
弯曲疲劳忍耐限度+73℉ASTM D-6714.5MPsi
弯曲疲劳忍耐限度+23℃ASTM D-67131.0MPa
弯曲降服强度+73℉ASTM D-79014.1MPsi
弯曲降服强度+23℃ASTM D-79097.2MPa
拉力冲击抵抗力+73℉ASTM D-1822100ft.lb/in2
拉力冲击抵抗力+23℃ASTM D-1822200kj/m2
扩散因数+73℉(+23℃)106HzASTM D-1500.005
负载下之变形2000psi@+122℉(14MPa@50℃)ASTM D-6210.5%
无切口冲击程度+23℃ASDM D-2561280j/m
无切口冲击程度+73℉ASDM D-25624ft.lb/in
断裂伸长率摩擦系数+73℉(+23℃)动态ThrustWasherTest30.35
摩擦系数+73℉(+23℃)静态ThrustWasherTest30.20
电气性能绝缘强度Short Time,90 milsASTM D-149500V/mil
绝缘强度Short Time,2.3mmASTM D-14919.7MV/m
电阻系数73℉(+23℃)0.2%H20ASDM D-2571015ohm-cm
绝缘系数+73℉(+23℃)102to106HzASTM D-1503.7
电弧抵抗力120mil(3.1mm)ASTM D-495220no trackingSec.

 